Scope
This standard applies to copper-zinc alloys (brass) pressure treated.
Stamps of usual brass
Brand and chemical composition of brass shall be as given in the table:
Mass fraction, % | |||||||||||
Mark | Pre — business | Item | The amount other elements |
The calculation of the probability density, g/cm3, |
Application example | ||||||
copper | lead | alt="GOST 15527−2004 Alloys copper-zinc (brass) pressure treated. Stamps (with Amendment, with the Change N 1)" class=doc-image-small v: shapes="_x0000_i1027">iron | 'alt="GOST 15527−2004 Alloys copper-zinc (brass) pressure treated. Stamps (with Amendment, with the Change N 1)" class=doc-image-small v: shapes="_x0000_i1028"> antimony | bismuth |
phosphorus |
zinc |
|||||
L96 | min. max. | 95,0 — 97,0 | - 0,03 |
- 0,1 |
- 0,005 |
- 0,002 |
- 0,01 |
The rest - |
- 0,2 |
8,9 | Sheets, wires, strips, pipes, rod, bars and wire for parts in electrical engineering, for medals and badges |
L90 | min. max. | 88,0 — 91,0 | - 0,03 |
- 0,1 |
- 0,005 |
- 0,002 |
- 0,01 |
The rest - |
- 0,2 |
8,8 |
|
L85 | min. max. | 84,0 — 86,0 | - 0,03 |
- 0,1 |
- 0,005 |
- 0,002 |
- 0,01 |
The rest - |
- 0,3 |
8,7 |
|
L80 | min. max. | 79,0 — 81,0 | - 0,03 |
- 0,1 |
- 0,005 |
- 0,002 |
- 0,01 |
The rest - |
- 0,3 |
8,7 |
Sheets, wires, strips, wire, art products, bellows, manometric tube, flexible pipes, musical instruments |
L70 | min. max. | 69,0 compared to 71.0 | - 0,05 |
- 0,07 |
- 0,002 |
- 0,002 |
- - |
The rest - |
- 0,2 |
8,5 |
Radiator tape, strips, pipes, heat exchangers, musical instruments, parts, produced by deep extraction |
L68 | min. max. | 67,0 — 70,0 | 0,03 | 0,1 | 0,005 | 0,002 | 0,01 | The rest - |
- 0,3 |
8,5 |
Wire mesh radiator tape, pipe for heat exchangers, parts, get deep |
L63 | min. max. | 62,0 — 65,0 | - 0,07 |
- 0,2 |
- 0,005 |
- 0,002 |
- 0,01 |
The rest - |
- 0,5 |
8,5 |
Sheets, wires, strips, tubes, rods, foil, wire, parts, get deep |
L60 | min. max. | 59,0 — 62,0 | - 0,3 |
- 0,2 |
- 0,01 |
- 0,003 |
- 0,01 |
The rest - |
- 1,0 |
8,4 |
Stamped parts, accessories |
In brass brand L68 intended for the production of special purpose products, the mass fraction of elements should not be more iron — 0,07%, antimony — 0,002%, phosphorus — 0,005%, arsenic — 0,005% sulphur — 0.002% of the (sum of other elements is 0.2%). The brass brands of l96, L90, L80, L70, L68, L63, L60 allowed mass fraction of Nickel up to 0.3% by mass fraction of copper, which do not take into account the amount of other elements. In brass all brands in coordination with the customer to determine the mass fraction of tin, aluminum, manganese and silicon, the values of which take into account the amount of other elements. In brass grade L70, used for the production of condenser tubes and heat exchangers allowed arsenic to 0.06% by mass fraction of copper, which do not take into account the amount of other elements. In brass brands L63, used in the food industry, the mass fraction of lead should not be more than 0.05%. For non-magnetic alloys, the mass fraction of iron should not be more than 0.03%. |
Supplier — the company Avecho offers various types of products from alloys of brass domestic and foreign production that meets the requirements of the standards. Products are offered at affordable prices from the manufacturer. Supplier guaranteed timely delivery at any address specified by the consumer.
The chemical composition and other special grades of brass
Mass fraction, % | |||||||||||||||
Mark | Pre — business | Item | The amount of other elements | The calculation of the probability density, g/cm, close — tional | An example of the prima tion | ||||||||||
copper | lead | iron | tin | Nickel | aluminium | cream — tions | antimony | bismuth | phosphorus | zinc |
|||||
LS74−3 | min. max. |
72,0- 75,0 |
2,4- 3,0 |
- 0,1 |
- - |
- - |
- - |
- - |
- 0,005 |
- 0,002 |
- 0,01 |
The rest - |
- 0,25 |
8,5 |
Tapes, strips, rods |
LS64−2 | min. max. |
63,0 — 66,0 | 1,5- 2,0 |
- 0,1 |
- - |
- - |
- - |
- - |
- 0,005 |
- 0,002 |
- 0,01 |
The rest - |
- 0,3 |
||
LS63−3 | min. max. | 62,0 — 65,0 | 2,4- 3,0 |
- 0,1 |
- 0,10 |
- - |
- - |
- - |
- 0,005 |
- 0,002 |
- 0,01 |
The rest - |
- 0,25 |
8,5 |
Tapes, strips, bars, rods, wire |
LS59−1V | min. max. | 57,0 — 61,0 | 0,8- 1,9 |
- 0,5 |
- - |
- - |
- - |
- - |
- 0,01 |
- 0,003 |
- 0,02 |
The rest - |
- 1,5 |
8,4 |
Bars |
LS59−1 | min. max. | 57,0 — 60,0 | 0,8- 1,9 |
- 0,5 |
- 0,3 |
- - |
- - |
- - |
- 0,01 |
- 0,003 |
- 0,02 |
The rest - |
- 0,75 |
8,4 |
Sheets, belts, strips, rods, profiles, tubes, wire, forgings |
LS58−2 | min. max. | 57,0 — 60,0 | 1,0- 3,0 |
- 0,7 |
- 1,0 |
- 0,6 |
- 0,3 |
- 0,3 |
- 0,01 |
- - |
- - |
The rest - |
- 0,3 |
8,4 |
Strip, bars, rods, wire |
LS58−3 | min. max. | 57,0 — 59,0 | 2,5- 3,5 |
- 0,5 |
- 0,4 |
- 0,5 |
- 0,1 |
- - |
- - |
- - |
- - |
The rest - |
- 0,2 |
Of 8.45 |
Bars |
LS59−2 | min. max. | 57,0 — 59,0 | 1,5- 2,5 |
- 0,4 |
- 0,3 |
- 0,4 |
- 0,1 |
- - |
- - |
- - |
- - |
The rest - |
- 0,2 |
8,4 |
Bars |
LZHS58−1-1 | min. max. | 56,0 — 58,0 | 0,7- 1,3 |
0,7- 1,3 |
- - |
- - |
- - |
- - |
- 0,01 |
- 0,003 |
- 0,02 |
The rest - |
- 0,5 |
8,4 |
Bars |
In leaded brass is allowed the mass fraction of Nickel is not more than 0.5%, the brass stamps LS59−1, LS59−1V, LS58−2 and LS58−3 — not more than 1% by mass fraction of copper, which is not taken into account in the total amount of other elements. In brass stamps LS59−1, the sum of the elements of tin and silicon should be not more than 0.5%. The brass of all brands it is possible to determine the mass fraction of tin, aluminum, manganese and silicon. In brass brand LS58−2 mass fraction of antimony in the manufacture of bars allowed no more than 0.1%. . |
Mass fraction, % | ||||||||||||||||||
Mark | Pre — business | Item | Amounts of other ele — men- tov |
The calculation of the probability density, g/cm, approx | Application example | |||||||||||||
copper | aluminium | mouse Yak |
jelly zo |
manganese | no- Kel |
cream — tions | tin | phosphorus | Bor |
Swee — Heff | sur — mA | vis — Mut | zinc |
|||||
LO90−1 | min. max. |
88,0- 91,0 |
- - |
- - |
- 0,1 |
- - |
- - |
- - |
0,2- 0,7 |
- 0,01 |
- - |
- 0,03 |
- 0,005 |
- 0,002 |
The rest - |
- 0,2 |
8,4 |
Tapes, strips, wire |
LO70−1 | min. max. | 69,0- 71.0 per |
- - |
- - |
- 0,07 |
- - |
- - |
- - |
1,0- 1,5 |
- 0,01 |
- - |
- 0,07 |
- 0,005 |
- 0,002 |
The rest - |
- 0,3 |
8,4 |
Sheets, strips, rods for instrumentation, tubing for condensers and heat exchangers |
Las 70−1-0,05 |
min. max. | 69,0 compared to 71.0 | - - |
0,02- 0,06 |
- 0,1 |
- - |
- - |
- - |
1,0- 1,5 |
- 0,01 |
- - |
- 0,07 |
- 0,005 |
- 0,002 |
The rest - |
- 0,3 |
8,4 | Pipe |
Las 70−1-0,04 |
min. max. | 69,0 compared to 71.0 | - - |
0,02- 0,04 |
- 0,07 |
- - |
- - |
- - |
1,0- 1,5 |
- 0,01 |
- - |
- 0,07 |
- 0,005 |
- 0,002 |
The rest - |
- 0,3 |
8,4 | Pipe |
LO62−1 | min. max. | 61,0 — 63,0 | - - |
- - |
- 0,10 |
- - |
- - |
- - |
0,7- 1,1 |
- 0,01 |
- - |
- 0,10 |
- 0,005 |
- 0,002 |
The rest - |
- 0,3 |
8,4 | Sheets, strips, rods for instrumentation, tubing for condensers and heat exchangers |
0,5 | ||||||||||||||||||
LKBO62- 0,2−0,04−0,5 |
min. max. | 60,5- 63,5 |
- - |
- - |
- 0,15 |
- - |
- - |
0,1- 0,3 |
0,3- 0,7 |
- - |
0,03 — 0,10 | - 0,08 |
- - |
- - |
The rest - |
Alu — mi — tions of 0.05 | 8,4 | Wire, rods |
LO60−1 | min. max. | 59,0- 61,0 |
- - |
- - |
- 0,1 |
- - |
- - |
- - |
1,0- 1,5 |
- 0,01 |
- - |
- 0,3 |
- 0,005 |
- 0,002 |
The rest - |
- 1,0 |
8,4 | Wire |
LOCKE 59−1-0,3 |
min. max. |
58,0- 60,0 |
- - |
- 0,01 |
- 0,15 |
- - |
- - |
0,2- 0,4 |
0,7- 1,1 |
- 0,01 |
- - |
- 0,1 |
- 0,01 |
- 0,003 |
The rest - |
- 0,3 |
8,4 | Wire, rods |
Lamsh 77−2-0,05 |
min. max. | 76,0- 79,0 |
1,7- 2,5 |
0,020- 0,06 |
- 0,1 |
- - |
- - |
- - |
- - |
- 0,01 |
- - |
- 0,07 |
- 0,005 |
- 0,002 |
The rest - |
- 0,3 |
8,4 | Pipe |
Lamsh 77−2-0,04 |
min. max. | 76,0- 79,0 |
1,7- 2,5 |
0,02- 0,04 |
- 0,1 |
- - |
- - |
- - |
- - |
- 0,01 |
- - |
- 0,07 |
- 0,005 |
- 0,002 |
The rest - |
- 0,3 |
8,4 | Pipe |
LA77−2 | min. max. | 76,0- 79,0 |
1,7- 2,5 |
- - |
- 0,07 |
- - |
- - |
- - |
- - |
- 0,01 |
- - |
- 0,07 |
- 0,005 |
- 0,002 |
The rest - |
- 0,3 |
8,3 | Seawater-resistant machinery parts, high-loaded valves |
LA77−2U | min. max. | 76,0- 79,0 |
1,7- 2,5 |
- - |
0,03- 0,10 |
0,03- 0,3 |
0,3- 1,0 |
0,03- 0,2 |
- - |
0,005- 0,02 |
- - |
- 0,07 |
- 0,005 |
- 0,002 |
The rest - |
- 0,1 |
8,3 | Pipe |
Lancz 75−2-2,5- 0,5−0,5 |
min. max. |
73,0- 76,0 |
1,6- 2,2 |
- - |
- 0,1 |
0,3- 0,7 |
2,0- 3,0 |
0,3- 0,7 |
- - |
- 0,01 |
- - |
- 0,05 |
- 0,005 |
- 0,002 |
The rest - |
- 0,5 |
8,3 | Strip, tubing |
1,4 | ||||||||||||||||||
LK75V | min. max. | 71.0 per- 78,0 |
- - |
- - |
- - |
- - |
- - |
0,25- 0,5 |
- - |
- - |
- - |
- 0,07 |
- - |
- - |
The rest - |
Tin 0,05 |
8,4 | Pipe |
L75mk | min. max. | 70,0- 76,0 |
- - |
- - |
0,03- 0,06 |
0,05- 0,15 |
0,1- 0,25 |
0,25- 0,5 |
- - |
0,005- 0,02 |
- - |
- 0,07 |
- 0,005 |
- 0,002 |
The rest - |
- 0,1 |
8,4 | Strip, tubing |
LMS 68−0,05 |
min. max. | 67,0- 70,0 |
- - |
0,02- 0,06 |
- 0,1 |
- - |
- - |
- - |
- - |
- 0,01 |
- - |
- 0,03 |
- 0,005 |
- 0,002 |
The rest - |
- 0,3 |
8,4 | Pipe |
LK62−0,5 | min. max. | 60,5- 63,5 |
- - |
- - |
- 0,15 |
- - |
- - |
0,3- 0,7 |
- - |
- - |
- - |
- 0,08 |
- 0,005 |
- 0,002 |
The rest - |
- 0,5 |
8,4 | Wire, rods |
The MESS 60−1-1 |
min. max. | 58,0- 61,0 |
0,7- 1,5 |
- - |
0,75- 1,50 |
0,1- 0,6 |
- - |
- - |
- - |
- 0,01 |
- - |
- 0,40 |
- 0,005 |
- 0,002 |
The rest - |
- 0,7 |
8,3 | Tubes, and rods for sliding bearings, shipbuilding and instrument engineering |
LAN 59−3-2 |
min. max. | 57,0- 60,0 |
2,5- 3,5 |
- - |
- 0,5 |
- - |
2,0- 3,0 |
- - |
- - |
- 0,01 |
- - |
- 0,1 |
- 0,005 |
- 0,003 |
The rest - |
- 0,9 |
8,2 | Rods, tubes |
Limc 59−1-1 |
min. max. | 57,0- 60,0 |
0,1- 0,4 |
- - |
0,6- 1,2 |
0,5- 0,8 |
- - |
- - |
0,3- 0,7 |
- 0,01 |
- - |
- 0,2 |
- 0,01 |
- 0,003 |
The rest - |
- 0,3 |
8,3 | Strip, pipe, bars, rods, wire |
Lmc58−2 | min. max. | 57,0- 60,0 |
- - |
- - |
- 0,5 |
1,0- 2,0 |
- - |
- - |
- - |
- 0,01 |
- - |
- 0,1 |
- 0,005 |
- 0,002 |
The rest - |
- 1,2 |
8,3 | Sheets, tapes, strips, bars, rods, wire for instrumentation |
In the complexly alloyed brass grades except LAN59−3-2, L75mk, LA77−2U, is allowed the mass fraction of Nickel up to 0.5%, which is not included in the total amount of other elements, and is counted as the mass fraction of copper. In brass brand Lmc58−2 at the customer’s request mass fraction of manganese is set in the range of 3.0%-4,0%. In brass LKBO62−0,2−0,04−0,5 mass fraction of boron content should be within the range of 0.03% to 0.10%, which does not include the amount of other elements. In brass brand LA77−2U mass fraction of iron less than 0.03% is not a rejection symptom. In brass brand Lamsh77−2-0,04 total mass fraction of phosphorus and arsenic should not be more than 0.04%. Manufacturer of brass stamps Lomsh70−1-0,04 permitted without the mass fraction of arsenic. |